Inconel 601 GC
1.Composition(wt%):
|
C
|
Cr
|
Ni
|
Fe
|
Cu
|
Mn
|
Al
|
Zr
|
N
|
Si
|
S
|
|
0.03-0.08
|
23.0
-
25.0
|
58.0
-
63.0
|
balance
|
≤1.0
|
≤1.0
|
0.8
-
1.7
|
0.07-0.25
|
0.02-0.07
|
≤0.50
|
≤0.03
|
2.Physical Properties
|
Density(g/cm3)
|
Melting point(℃)
|
Curie temperature (℃)
|
Specific heat capacity
J/(Kg*℃)
|
|
8.11
|
1301~1368 ℃
|
-196
|
480
|
3.Mechanical Properties
Tensile properties at room temperature
|
Material Name
|
Tensile strength(MPa)
|
Yield strength(MPa)
|
Elongation %
|
|
Inconel 601 GC
|
585-690
|
205-405
|
55-35
|
High temperature creep properties
|
Temperature(℃)
|
Rupture strength(MPa)
|
Time(h)
|
|
980
|
28
|
40
|
|
1095
|
14
|
60
|
|
1175
|
6.9
|
40
|
|
1175
|
5.5
|
60
|
|
1175
|
4.1
|
160
|
4.Characteristics
INCONEL alloy 601GC is a grain controlled version of INCONEL alloy 601 (UNS N06601).
Zirconium and nitrogen in INCONEL alloy 601GC act to inhibit grain growth during
exposure to high temperatures. Grain size stability is an important factor in obtaining
optimum performance and service life at high temperatures.
5.Applications
1).Seam-welded roller tubes in roller-hearth furnaces
2).Production of glazed ceramic tiles. |